EverflonTM FEP 4610
FEP Machining Speeds, Feeds and Tools
Review cutting speed, feed, cooling, tool geometry and workpiece support.
Machining
Machining FEP stock is useful for tight tolerances, complex shapes or a few prototypes. Turning, facing, boring, drilling, threading, tapping, reaming and grinding are applicable; the source says specialized machinery is unnecessary.
FEP is soft yet resilient and waxy yet tough. The source compares its cutting feel to brass and tool-wear effect to stainless steel. Skilled machining may achieve ±0.001 in and, with special care, ±0.0005 in (±0.0254 and ±0.0127 mm), not a universal tolerance promise.
Choosing Working Speeds
Low thermal conductivity retains cutting heat, which can dull tools and overheat resin. Cooling matters especially above 150 m/min. The source compares expansion to nearly ten times that of metals; local heat may cause overcuts, undercuts or tapered holes.
Finish turning at 60–150 m/min generally needs no flood coolant. Higher speed may suit low feed or roughing but requires heat removal.
| Item | Metric | US units / notes |
|---|---|---|
| Finish-turning surface speed | 60–150m/min | 200–500fpm |
| Feed per revolution | 0.05–0.25mm/rev | 0.002–0.010 in/rev; for the stated speed range |
| High-speed example | 240m/min | 800 fpm; reduce feed for finishing |
| Depth of cut | 0.005–6.3mm | 0.0002–0.25in |
| Drilling feed | 0.13–0.23mm/rev | 0.005–0.009in/rev |
| Coolant | Water : water-soluble oil = 10:1–20:1 | Source ratio |
Intermittent drilling can help transfer heat into coolant. Surface speed is not spindle rpm, and feed per revolution is not feed per minute.
Tool Geometry and Use
Standard tools can be used; shaping them for FEP helps heat control and quality. Boring tools usually use the higher listed angles.
| Item | Source term | Angle |
|---|---|---|
| Top rake | Top rake | 0–15°, positive rake |
| Side rake and side angle | Side rake and side angle | 0–15° |
| Front or end rake | Front or end rake | 0.5–10° |
Dull tools may pull stock out of line and remove excess material; unsuitable edges may compress it and undercut. Keep edges sharp, especially for filled materials. Stellite-type or carbide tips reduce resharpening. A small nose radius partly compensates wear; drills need deep polished flutes.
Support long slender stock. Continuous curled chips must be guided away to avoid wrapping, coolant obstruction or displacement. The source mentions momentary tool withdrawal on automatic screw machines.
Source data, charts and compliance statements concern another manufacturer’s reference material. Renaming a grade does not establish equivalence or measured performance for Everflon FEP 4610. Curves are approximate illustrations, not engineering input. · Product and Properties Handbook: Forming And Fabrication; Choose Correct Working Speeds; Properly Shape And Use Tools