Creep and Cold Flow
Continued deformation under sustained load is creep or cold flow. Metals behave similarly at elevated temperature, but plastics may deform significantly at or below room temperature. Stress, time and temperature are key variables.
Initial strain occurs immediately on loading, followed by continued deformation, usually at a decreasing rate. Creep can be measured in tension, compression or flexure. Flexure is easier to measure; tensile and compressive data are often more directly useful for design.
Figures 10–13 use different tensile stresses at different temperatures; curve heights alone do not isolate temperature effects. Figures 14–15 concern compression.
Approximate source redraw; not measured 4610 data.
Approximate source redraw; not measured 4610 data.
Approximate source redraw; not measured 4610 data.
Approximate source redraw; not measured 4610 data.
Approximate source redraw; not measured 4610 data.
Approximate source redraw; not measured 4610 data.
Apparent Modulus of Elasticity
Apparent modulus accounts for initial and time-dependent creep strain. Define acceptable strain over the required service life; shorter loading duration generally permits a higher apparent modulus and allowable stress.
Use dimensionless strain. The source example at 23°C and 1,000 psi gives about 66,700 psi for initial strain 0.015 and 50,000 psi for total strain 0.02 after 200 h. Extrapolation to one year uses 0.025, giving 40,000 psi.
| Time | Stress | Total strain | Calculated result |
|---|---|---|---|
| Initial | 1,000 psi | 0.015 | Approx. 66,700 psi |
| 200 h | 1,000 psi | 0.020 | 50,000 psi |
| One year, source extrapolation | 1,000 psi | 0.025 | 40,000 psi |
Plotting apparent modulus against time supports creep assessment. Some source curves level off; whether later creep can be neglected depends on allowable deformation and service conditions.
Stress Relaxation
Cold-flowing flange gaskets can undergo stress relaxation. Lined valves or tees may use extended lining as a gasket. Cold flow between flange faces can reduce bolt preload and cause leakage.
The source discusses retightening during the first day. Actual retightening must follow equipment and gasket instructions, not a universal procedure. Figures 16–17 show decreasing stress at constant strain.
Approximate source redraw; not measured 4610 data.
Approximate source redraw; not measured 4610 data.
Source data, charts and compliance statements concern another manufacturer’s reference material. Renaming a grade does not establish equivalence or measured performance for Everflon FEP 4610. Curves are approximate illustrations, not engineering input. · Product and Properties Handbook: Creep And Cold Flow; Apparent Modulus Of Elasticity; Stress Relaxation