EverflonTM FEP 4610
FEP Absorption, Permeability and Weathering
Compare absorption and transmission, with film thickness and test conditions in view.
Absorption
Most plastics absorb small amounts of contacting substances into intermolecular spaces without necessarily reacting. Slight weight gain and sometimes discoloration can result.
The source reports very low absorption: virtually none for common acids and bases up to 200°C over one year, generally less than 1% weight gain from long high-temperature solvent exposure, and typical moisture uptake below 0.01% at ambient conditions. This does not validate every medium.
Permeability
Many gases and vapors pass through the source FEP more slowly than other thermoplastics. Total transmission generally rises with temperature, pressure and area and falls with thickness. Check normalization when comparing data.
| Gas | cc/(m²·24 hr·atm) |
|---|---|
| Carbon dioxide | 25.9 × 10³ |
| Hydrogen | 34.1 × 10³ |
| Nitrogen | 5.0 × 10³ |
| Oxygen | 11.6 × 10³ |
Conditions: 1 mil (about 25 μm), 25°C, ASTM D1434-75. Multiply by 0.0645 for a per-100-in² basis.
Table 8 uses 1 mil film and modified ASTM E96. Each medium is at its vapor pressure at the stated temperature.
| Medium | °C | °F | g/(m²·d) | g/(100in²·d) |
|---|---|---|---|---|
| Acetic acid | 35 | 95 | 6.3 | 0.41 |
| Acetone | 35 | 95 | 14.7 | 0.95 |
| Benzene | 35 | 95 | 9.9 | 0.64 |
| Carbon tetrachloride | 35 | 95 | 4.8 | 0.31 |
| Ethyl acetate | 35 | 95 | 11.7 | 0.76 |
| Ethanol | 35 | 95 | 10.7 | 0.69 |
| F-12 refrigerant (source medium) | 23 | 73 | 372 | 24 |
| Hexane | 35 | 95 | 8.7 | 0.56 |
| Hydrochloric acid | 25 | 77 | <0.2 | <0.01 |
| Red fuming nitric acid | 25 | 77 | 160 | 10.5 |
| 50% sodium hydroxide | 25 | 77 | <0.2 | <0.01 |
| 98% sulfuric acid | 25 | 77 | 2 × 10⁻⁴ | 1 × 10⁻⁵ |
| Water | 39.5 | 103 | 7.0 | 0.40 |
Water Vapor Transmission
Figure 24 relates water-vapor transmission to thickness at 40°C (104°F), modified ASTM E96. Values are averages, not specifications. Multiply per-100-in² values by 15.5 for a per-m² basis.
Approximate source redraw; not measured 4610 data.
Weathering
After 25 years outdoors in Florida, the source material was essentially unchanged: tensile strength was unaffected and elongation apparently decreased somewhat but remained high. This is not a 4610 exposure test or service-life guarantee.
Source data, charts and compliance statements concern another manufacturer’s reference material. Renaming a grade does not establish equivalence or measured performance for Everflon FEP 4610. Curves are approximate illustrations, not engineering input. · Product and Properties Handbook: Absorption; Permeability; Water Vapor Transmission; Weathering